APPLICATION MANUAL OF MICROCEMENT
Materials needed:
The primer Displex AGMA bridge or CH
Corrector Mortar Media
thick microcement. (1 kg m2 layer) (recommended 2 coats may be more)
fine microcemento . (300 gr. M2 and coat, 2 coats minimum recommended max. 3)
Color pigment. (1 Bottle of pigment per cube)
Displex 3342 (47% for fine and 30 for the bulk)
Dur Pavilac or Pavilac Hydrowax
NO NEED FIBERGLASS MESH, THE FIBERGLASS MESH IN A MICROCEMENT
SERVES ONLY TO COVER MICROCEMENTO DEFICIENCY QUALITY.
Tools needed:
Clean container for mixing (You can use these cubes)
1 flexible metal trowel
1 flexible plastic trowel (like those used in the drywall putty)
Simple mixer (Mixer stem common large)
A drill rod for mixing paint (for steel)
Pasaceras sponge or short nap roller microfiber
Broom, dustpan and vacuum
Masking tape (to make all the ends and get rid of every day)
Grit 40 or 60 (for thickness)
Grit 220 or 240 (for steel)
Grit 400 or 600 (for sanding the premier if he had painted before the final)
Preparation of base support
On walkable ground (mostly because the workability of the stickiness of the material)
We will use only AGMA CH. Depending on the porosity of the material may be diluted to CH AGMA part of three drinking water.
Single wall or vertical faces little or no porous employ the DISPLEX
PUENTE, for porous despite being vertically using the AGMA CH.
The solution in water from the AGMA CH, it is possible for their apparent concentration of additives,
but depending on the porosity of the material must be diluted in about proportion
to facilitate its maximum penetration. Only non-porous materials should be used in
pure state.
In concrete, first of all, we will sand clean, milling the surface if necessary to fix the
tips and imperfections to avoid getting sufficient flatness and to avoid consumption
unnecessary bulk. Failure to meet the flatness, apply at least AGMA both hands and apply self-leveling mortar CH Leveland. (This mortar leveling can be applied by hand or machine and provides indoor and outdoor
also that neither cracks or breaks up)
The Displex bridge or if the AGMA CH, favor tighter media such as
mortar, plaster ... and materials that do not require this hardening does not provide troweling, (welcome to apply the bulk product in a mirror without primer some and leave it sets so just 12 hours of the 28 days established for setting chemicals are of the brand they are, see the adherence of our case material only) also managed to avoid dehydration is to apply the material.
 |
 |
For the application of questionable reliability-based media in terms of reactions or compositions are existing or applied for the same applicator microcemento, use after correcting primer mortar carriers. (It has less overhead additive that can be applied in mixed horizontal supports between 40 and 50% resin of which comes with the product that can be applied by roller, so two coats of this material in any format will simplify the work by providing a savings important in labor) can be applied by trowel in thicknesses of 1 mm per layer with a mixture of 30 to 35%.
This correction will always be used after priming, and also to avoid transmission slot in the base microcemento exists for its grip and absorption of expansion movements also impervious to prevent capillary moisture even negative pressure in case of swimming pools. (has health certificate for use in deposit waterproofing devices)
On brick, mortar excel first (obviously, to work this material, all the walls must be properly teacher, to avoid an intake unnecessary.. may be filled with coarse material but consumption would be costly.
On firm and even natural wood laminated flooring, remove waxed coatings only if
and if not varnished apply a coat of AGMA-CH diluted (1 part 1 part CH AGMA
of water even if it is deemed more) and at least one hand over AGMA CH in pure form or
Concentrate. (you can insert another intermediate hand with a solution). If they are
varnished and choose not to remove them (they are not waxed) CH AGMA apply
when pure and dry in an hour or two pair of hands apply a mortar offset (the first hand roll and the next level with mixtures explained above).
On firm and even natural wood laminated flooring, remove waxed coatings only if
and if not varnished apply a coat of AGMA-CH diluted (1 part 1 part CH AGMA
of water even if it is deemed more) and at least one hand over AGMA CH in pure form or
Concentrate. (you can insert another intermediate hand with a solution). If they are
varnished and choose not to remove them (they are not waxed) CH AGMA apply
when pure and dry in an hour or two pair of hands apply a mortar
offset (the first hand roll and the next level with mixtures explained
above) About mortar finishings, mortar will always implement media for corrector transmitted from the firm to avoid problems.
Taping sockets and divisions if any.
We recommend deleting the old baseboards and skirting combined with glass, stone
or natural wood.
Application of Thick Microcement Use a flexible metal trowel yesaire, for a perfect flat
against the base surface.
Apply at least two coats of thick with DISPLEX Microcement Pavicon 3342 (with a
resin mixture of 30 to max. 33% (depending on weather) and thus, in 10 kg
dust exactly 3 liters of resin), on a perfectly flat (finished or perfectly smooth, and primed using the steps explained in
before).
 |
Fine beforehand, can be pigmented to help too much fine sanding microcement discovered or disguise the bulk (mixing the same for all products, a pigment for a cube).
Application of MC with sander thickness less than 300 mm in diameter, either circular, hand giraffe actions and even hand actions. (the latter is only possible if the sanding is done
before total drying).
Apply a surface MC Thick metal trowel giving a flexible yesaire thickness between 0.5 and 1 mm per layer (to which the arid) as sanding, with this type of
machinery, is less intense, so the thickness may also be less. (Consumption 1 kg / m 2 and layer) sanding with grit 40 or 60 and the corresponding vacuum. Sand when surface is at a point of being neither tender (because it
will be difficult to sand) We recall again that the sand will never be when the material is tender but important to avoid doing so when the material is dry, it can be quite costly, Given the hardness of the material (if the material was dry and out large surface which stay by sand and impossible, it could be sanded with 80 grit disc hydrocarbon would be preferable or even give a worn hand of extra thickness.) Open time setting of the material is extended for this reason, we always provide workability.
 |
For hand sanding can help a Styrofoam cork with sandpaper (the swirling typically used in mortar lucid common) can only be sanded so if the dried material is not 100%, otherwise it is impossible for a lot of will used.
Application of MC thickness sanding machine with professional rotating more than 40 cm. of
diameter.
Each layer (with thickness MC) will be between 1.5 and max. 2 mm. thick, for after the sanding, achieve excellent flatness. The professional sanding machine diameter circular
greater than 40 cm, sanding wear will be higher, leaving a final score of 1 mm
layer thickness. (The flatness with this system is optimal) (consumption between 2 and 2.5 kg/m2 layer).
After applying the appropriate thickness of MC Thick, sand with 40 grit sanding to
achieve ideal flatness of the surface and then vacuum between coats.
Application of Fine Microcemento with 220 grit sanding with rotating machine or other lower to 300 mm in diameter, either hand or giraffe:
 |
 |
After verifying the excellent flatness we have managed to lock
with the fine for mixing the resin fine Displex 3342 at a rate of between
43 and 47%.
43 will be used for ceilings, walls and 47- 45 for floor, more than anything to avoid the
dripping or sagging ground spotted the material in the flat. Mix 47% will be in 10 kg of fine powder resin 4.7-liter will be 3342.
As a pigment for a bucket is full, we will estimate the resin powder kg
use (meaning we consume about 300 grams per m2 and coat each layer as it will that in the aggregate and can be perfectly max. a tenth of a mm).
Once the resin in the bowl, add the pigment weight equivalent, we will beat
3342 resin with a drill mixer to beat new paint stem or impeccable (so you do not release impurities since the touch is like taco powder) and once While you add the powder dissolved precise about the proportion calculated.
(Solid pigment, from the pigments used in our monolayer of facades,
that with our experience since 1962 we know what type of pigment is the
necessary to avoid fading, and this converted after mixing of additives with agitators
mechanical and other processes such as screened, transformed into liquid form so that
not suffer scratches on the application brought on by certain pigments diluted)
Use a flat flexible plastic such as drywall applicators (we
use a flexible flat with rounded edges to prevent burrs, except for make brackets) to achieve the highest perfection at the time of application.
 |
(We recommend that the last application of thin trowel is new, to avoid streaks and
small indentations, the penultimate application can be plain that we had used in another
application as the last, and for the first hand, in turn use that on another occasion
use as penultimate) If in this case uses ultra flat flexible metal or flexible
finished water will get considerably more pronounced but not if the waters
material if not for wear or sanding it flat on the material itself caused by the
have micro abrasion. (another type of finish would be widely used in various areas of
which are not in favor because it scratching the confusion level with the waters of the
material).
For the sand were used for basic reasons of the aggregate, a minimum of 220 sandpaper and max. 260 (220 recommended by the grain that does not draw a line to dry and sanding more to help
other finer).
The sanding should be when you see 100% dry material and the setting (which has nothingto do with out) is controlled to allow time for sanding comfortably.
A good application is fine as it is hardly necessary to sand, which sand is used
"As a cloth to remove dust."
It is important to know that the fine is not to level any bumps, should go to tested with
that the aggregate against the bottom bracket, so it is important not to make fine if the base or
thickness is not well planimeter.
Machine sanding application with professional press over grain diameter 40mm
220: Apply at least 2 or 3 layers of up to 1 or 1.5 mm thick each, and sand with
a circular sander 220 grit. After each grinding, we will always further
suction. (To both layer thickness, we make the mixture too thick, between
40 to 43% max.).
Each layer (with fine MC) will be between 1 and 1.5 mm. thickness, this thickness being necessary minimum, because the sanding, in this case, professional buffing machine will be circular with large diameter for excellent flatness and therefore, this type of machine, the wear will be higher, with a maximum bottom layer of 0.5 to 1mm
thick. (Consumption 1 to 2kg / m 2 and layer).
Pavilac application (this process can be replaced by Pavilac - Dur) (application to roll
short hair lacquer or spray).
NEVER REPLACE THIS PROCESS BY A WAX.
Do not substitute PAVILAC PROCESS by the wax, as a result, there would be wear
few weeks by washing (with or without soap) and would be affected with microcemento
any spills.
The Pavilac is a product of one-component water lacquer. (Use a roller or spray
between 50 and 150 g m2 and consumption clearly layer by the applicator).
The Pavilac, seep into all layers. After drying, crystallize, harden, clog
pores and be a very hard surface, so that in the second last match pores
covered, and the third body will get enough to terminate the application.
Optimal hardness 7 days, walkable in 6 hours drying time between layers 6 hours despite being dry to the touch.
Application of Pavilac Dur (two-component solvent) (application to hair lacquer roller
short or gun) This material is of the utmost quality but suitable only for professionals. (The company is not responsible for the misuse of materials by lack of implementation or adaptation
it).
Any product solvent whatever their brand, it must take account of their compatibility, it is important to have a humidity control, ventilation, that kind of application will be placed, temperature ...
It is important because moisture softens the dry product to solvent while (could
soften the system but would stiffen but multiplied by 30 times hardened)
It is important because the temperature below 15 degrees and above 30 as
any two-component compound may affect its catalysts.
Ventilation is important for their drafts, as these can cause dry superficial part before the lower and thus the solvents do not go out and harm the system hardening (delayed).
Coater's work life has been a professional work, it is important to at least consider
these points to facilitate the work or learning.
professional mask recommended .
Combining the pigments base, the customer has the possibility to get many colors to your liking, finished in gloss, matte or satin finish.
No matter the destination or location of the work to agree on a particular color, because we can stick to any kind of color reference as any professional decorative coatings or paints, it is easy to find among his tools use a color chart (either RAL, Pantone or NCS natural color).
However, some colors have stock listed as standard.
IMPORTANT:
Why do the pigments are liquid?
In BCP, we have been manufacturing since 1962 resins and additives, being almost 50 years we have been producing monolayers and colored cementitious products inside and out.
The pigment does not fade, do not fade and the quality of our product line aims to offer is an initial source of pigment solid state. (Dust) within the range of solid pigments, we work with the best quality. (Thousands of works of monolayer services throughout our history behind us)
For us it is very easy to mix the necessary proportion of dust in the cube have micro, but it is not properly correct for several reasons:
The pigment dilution takes quality (can appear flat when passing tear caused by a grain of undissolved pigment and causes a wake bay shooting mode to decomposition) Understand that dissolve easily but 80% of the pigment , and with effort 90 to 95%, only 1% that does not dissolve and ruin the application (10 / 12 lines per m2)
If the pigment was in liquid water as those sold in the market by dissolving pigmentosa brilliantly, but using liquid pigment, remember that it is not the same quality, and also adversely affects the mix microcemento, and the pigment-based liquid is water and if the mixture needs of 10 kg have micro (MC) or micro-concrete (MH), 4 liters of resin, pigment if it takes 1 liter of water, only enter the 3 liters of resin mixture, so that the hardness is affected by 20%. Besides being pigments that resist radiation or alkalinity.
BCP, the pigment used in the solid state to liquid transformed in this way, the same type of high-quality pigment for mortar and monolayers, using a chemical process at the atomic level desfracmentamos pigments and then additive alloys, we transform the pigment in a liquid state, where this process is added to the mix additive value of hardness and plasticity necessary.
D The mixture is provided a container of pigment by a container of any product in our dust, so each product has a certain type of Kg.
If on the other hand you want to add pigment tilts grams, is quite simple:
1 -. although the pigment and the pigment weight divided by the MC or MH Kg has raw (coming grams per kilogram of pigment MC or MH)
2 -. select few kg of MC or MH, you put utilizar.y grams per kg previously calculated for each kg of MC or MH desired.
Never have a different tone with this practice, but if you want more complicated formats can ask young as 5 or 10 pounds and make the mixture 100% 100% pigment dust.
Feel Free to speak with our technical advisors; Telf: 0034 969 100 100 or send us a email: tecnico@bcpfabrica.com
We offer one option to get the right tools to apply acorrectly, please visit: